Trang 1Handbook of Comparative World Steel Standards
5.9 Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures
5.9.2A Chemical Composition of Austenitic Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures (Continued)
Weight, %, max, Unless Otherwise Specified Standard
Designation Grade, Class, Type, Symbol or Name Number Steel Number UNS C Mn Si P S Cr Ni Mo Others
ASTM A 213/A 213M-03a TP304H - S30409 0.04-0.10 2.00 0.75 0.040 0.030 18.0-20.0 8.00-11.0 - -
Trang 2ASTM A 213/A 213M-03a TP310H - S31009 0.04-0.10 2.00 0.75 0.040 0.030 24.00-26.00 19.0-22.00 - -
BS 3605-2:1992 AMD 1:1997
316S33 - - 0.070 2.00 1.00 0.04 0.03 16.50-18.50 11.00-14.00 2.50-3.00 - DIN 17457:1985 X 5 CrNiMo 17 12 2 1.4401 - 0.07 - - - - 16.5-18.5 10.5-13.5 2.0-2.5 -
Trang 3Handbook of Comparative World Steel Standards
5.9 Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures
5.9.2A Chemical Composition of Austenitic Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures (Continued)
Weight, %, max, Unless Otherwise Specified Standard
Designation Grade, Class, Type, Symbol or Name Number Steel Number UNS C Mn Si P S Cr Ni Mo Others
TS 60 - - 0.07 2.00 1.00 0.045 0.030 16.00-18.50 11.00-14.00 2.00-2.50 - ISO 2604-II:1975
TS 61 - - 0.07 2.00 1.00 0.045 0.030 16.00-18.50 11.00-14.50 2.50-3.00 -
TW 60 - - 0.07 2.00 1.00 0.045 0.030 16.00-18.50 10.50-14.00 2.00-2.50 - ISO 2604-V:1978
TW 61 - - 0.07 2.00 1.00 0.045 0.030 16.00-18.50 11.00-14.50 2.50-3.00 - ASTM A 213/A 213M-03a TP316L - S31603 0.035 2.00 0.75 0.040 0.030 16.0-18.0 10.0-15.0 2.00-3.00 -
BS 3605-2:1992 AMD 1:1997
316S13 - - 0.030 2.00 1.00 0.04 0.03 16.50-18.50 11.50-14.50 2.50-3.00 - DIN 17457:1985 X 2 CrNiMo 17 13 2 1.4404 - 0.030 - - - - 16.5-18.5 11.0-14.0 2.0-2.5 -
TU Z 2 CND 18 14 - - 0.030 2.00 1.00 0.020 0.015 17.00-18.50 13.00-16.00 2.20-3.00 - AFNOR NF A 49-247:1981 TS Z 2 CND 17-12 - - 0.030 2.00 1.00 0.040 0.030 16-18.0 10.5-13.00 2.00-2.40 -
TS 57 - - 0.03 2.00 1.00 0.045 0.030 16.00-18.50 11.00-14.00 2.00-2.50 - ISO 2604-II:1975
TS 58 - - 0.03 2.00 1.00 0.045 0.030 16.00-18.50 11.50-14.50 2.50-3.00 -
TW 57 - - 0.03 2.00 1.00 0.045 0.030 16.00-18.50 11.00-14.00 2.00-2.50 - ISO 2604-V:1978
TW 58 - - 0.03 2.00 1.00 0.045 0.030 16.00-18.50 11.50-14.50 2.50-3.00 -
Trang 4ASTM A 213/A 213M-03a TP316LN - S31653 0.035 2.00 0.75 0.040 0.030 16.0-18.0 11.0-14.0 2.00-3.00 0.10-0.16
X3CrNiMoN17-12 - - 0.030 2.00 0.75 0.040 0.015 16.0-18.0 11.0-13.0 2.5-3.0 N 0.12-0.20 ASTM A 213/A 213M-03a TP316H - S31609 0.04-0.10 2.00 0.75 0.040 0.030 186.0-18.0 11.0-14.0 2.00-3.00 -
JIS G 3463:1994 SUS316TiTB - - 0.08 2.00 1.00 0.040 0.030 16.00-18.00 10.00-1400 2.00-3.00 Ti 5 x C min
Trang 5Handbook of Comparative World Steel Standards
5.9 Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures
5.9.2A Chemical Composition of Austenitic Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures (Continued)
Weight, %, max, Unless Otherwise Specified Standard
Designation Grade, Class, Type, Symbol or Name Number Steel Number UNS C Mn Si P S Cr Ni Mo Others
ASTM A 213/A 213M-03a TP317 - S31700 0.08 2.00 0.75 0.040 0.030 18.0-20.0 11.0-14.0 3.00-4.00 -
ASTM A 409/A 409M-01 TP321 - S32100 0.08 2.00 1.00 0.045 0.030 17.0-20.0 9.00-12.0 - Ti 5 x C to 0.70
JIS G 3459:1997 SUS321TP - - 0.08 2.00 1.00 0.040 0.030 17.00-19.00 9.00-13.00 - Ti 5 x C min
JIS G 3463:1994 SUS321TB - - 0.08 2.00 1.00 0.040 0.030 17.00-19.00 9.00-13.00 - Ti 5 x C min
JIS G 3467:1988 SUS 321 TF - - 0.08 2.00 1.00 0.040 0.030 17.00-19.00 9.00-13.00 - Ti 5 x C min
JIS G 3468:1994 SUS321 - - 0.08 2.00 1.00 0.045 0.030 17.00-19.00 9.00-13.00 - Ti 5 x C min
Trang 6ASTM A 213/A 213M-03a TP321H - S32109 0.04-0.10 2.00 0.75 0.040 0.030 17.0-20.0 9.00-13.0 - Ti 4 X C-0.60
ASTM A 249/A 249M-03 TP321H - S32109 0.04-0.10 2.00 1.00 0.045 0.030 17.0-19.0 9.00-12.0 - N 0.10; Ti 5 x (C+N) to 0.70 ASTM A 312/A 312M-03 TP321H - S32109 0.04-0.10 2.00 1.00 0.045 0.030 17.0-19.0 9.0-12.0 - Ti 5 x C to 0.60
ASTM A 376/A 376M-02a TP321H - S32109 0.04-0.10 2.00 0.75 0.040 0.030 17.0-19.0 9.00-13.0 - Ti 4 x C to 0.70
ASTM A 358/A 358M-01 347 - S34700 0.08 2.00 0.75 0.045 0.030 17.0-19.0 9.0-13.0 - Cb 10 x C to 1.00
ASTM A 376/A 376M-02a TP347 - - 0.08 2.00 0.75 0.040 0.030 17.0-19.0 9.00-13.0 - Cb 10 x C to 1.10
ASTM A 409/A 409M-01 TP347 - S34700 0.08 2.00 1.00 0.045 0.030 17.0-19.0 9.00-12.0 - (Cb+Ta) 10 x C to 1.10
JIS G 3459:1997 SUS347TP - - 0.08 2.00 1.00 0.040 0.030 17.00-19.00 9.00-13.00 - Nb 10 x C min
JIS G 3463:1994 SUS347TB - - 0.08 2.00 1.00 0.040 0.030 17.00-19.00 9.00-13.00 - Nb 10 x C min
JIS G 3467:1988 SUS 347 TF - - 0.08 2.00 1.00 0.040 0.030 17.00-19.00 9.00-13.00 - Nb 10 x C min
JIS G 3468:1994 SUS347 - - 0.08 2.00 1.00 0.045 0.030 17.00-19.00 9.00-13.00 - Nb 10 x C min
Trang 7Handbook of Comparative World Steel Standards
5.9 Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures
5.9.2A Chemical Composition of Austenitic Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures (Continued)
Weight, %, max, Unless Otherwise Specified Standard
Designation Grade, Class, Type, Symbol or Name Number Steel Number UNS C Mn Si P S Cr Ni Mo Others
ASTM A 213/A 213M-03a TP347H - S34709 0.04-0.10 2.00 0.75 0.040 0.030 17.0-20.0 9.00-13.0 - Cb+Ta 8 X C -1.0
JIS G 3467:1988 NCF 800H TF - - 0.05-0.10 1.50 1.00 0.030 0.015 19.00-23.00 30.00-35.00 - Cu 0.75; Al 0.15-0.60; Ti 0.15-0.60
- - N08367 0.030 2.00 1.00 0.040 0.030 20.0-22.0 23.5-25.5 6.0-7.0 N 0.18-0.25; Cu 0.75 ASTM A 249/A 249M-03
- - N08926 0.020 2.00 0.50 0.030 0.010 19.0-21.0 24.0-26.0 6.0-7.0 N 0.15-0.25; Cu 0.50-1.50 ASTM A 312/A 312M-03 - - N08926 0.020 2.00 0.50 0.030 0.010 24.0-26.0 19.0-21.0 6.0-7.0 N 0.15-0.25; Cu 0.50-1.50
- - N08367 0.030 2.00 1.00 0.040 0.030 20.00-22.00 23.50-25.50 6.00-7.00 N 0.18-0.25; Cu 0.75 ASTM A 688/A 688M-03
- - N08926 0.020 2.00 0.5 0.03 0.01 19.00-21.00 24.00-26.00 6.0-7.0 N 0.15-0.25; Cu 0.5-1.5 JIS G 3463:1994 SUS836LTB - - 0.030 2.00 1.00 0.040 0.030 19.00-24.00 24.00-26.00 5.00-7.00 N 0.25
Trang 8MPa MPa
ASTM A 358/A 358M-01 304 - S30400 H, HT, HT-O
ASTM A 409/A 409M-01 TP304 - S30400 H, HT, HT-O
T: 55 J at RT DIN 28180:1985 X 5 CrNi 18 10 1.4301 - SA & Q ≤ 50 - 195 - 500-700 - 40 L; 35 T L: 85 J at RT
T: 55 J at RT DIN 28181:1985 X 5 CrNi 18 10 1.4301 - SA & Q ≤ 50 - 195 - 500-720 - 40 L; 35 T 85 J at RT, L
55 J at RT, T AFNOR NF A 49-217:1987 TU Z 6 CN 18 09 - - HF + CR + Q (HY) - - 200 - 490-740 - 45 90 HRB max
Trang 9Handbook of Comparative World Steel Standards
5.9 Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures
5.9.2B Mechanical Properties of Austenitic Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures (Continued)
Thickness Yield Strength, min Tensile Strength, min Standard
Designation Grade, Class, Type, Symbol or Name Number Steel Number UNS Heat Treatment Product Form/ t, mm t, in N/mm 2 or
2 or
Elongation, min, % Other
T: 55 J at RT AFNOR NF A 49-217:1987 TU Z 2 CN 18 10 - - HF + CR + Q (HY) - - 175 - 470-720 - 45 90 HRB
DIN 17457:1985 X 2 CrNiN 18 10 1.4311 - SA & Q ≤ 50 - 270 - 550-760 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT DIN 17458:1985 X 2 CrNiN 18 10 1.4311 - SA & Q ≤ 50 - 270 - 550-760 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT AFNOR NF A 49-217:1987 TU Z 2 CN 18 10 AZ - - - - - 240 - 550-800 - 40 -
NOTE: This section continued on next page
Trang 10AFNOR NF A 49-217:1987 TU Z 1 CNS 18 15 - - HF + CR + Q (HY) - - 220 - 540-740 - 40 -
Trang 11Handbook of Comparative World Steel Standards
5.9 Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures
5.9.2B Mechanical Properties of Austenitic Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures (Continued)
Thickness Yield Strength, min Tensile Strength, min Standard
Designation Grade, Class, Type, Symbol or Name Number Steel Number UNS Heat Treatment Product Form/ t, mm t, in N/mm 2 or
2 or
Elongation, min, % Other
Trang 12MPa MPa
ASTM A 358/A 358M-01 316 - S31600 H, HT, HT-O
ASTM A 409/A 409M-01 TP316 - S31600 H, HT, HT-O
T: 55 J at RT DIN 17457:1985 X 5 CrNiMo17 13 3 1.4436 - SA & Q ≤ 50 - 205 - 510-710 - 40 L; 35 T L: 85 J at RT
T: 55 J at RT DIN 17458:1985 X 5 CrNiMo17 13 3 1.4436 - SA & Q ≤ 50 - 205 - 510-710 - 40 L; 30 T L: 85 J at RT
T: 55 J at RT DIN 28180:1985 X 5 CrNiMo 17 12 2 1.4401 - SA & Q ≤ 50 - 205 - 510-710 - 40 L; 30 T L: 85 J at RT
T: 55 J at RT DIN 28181:1985 X 5 CrNiMo 17 12 2 1.4401 - SA & Q ≤ 50 - 205 - 510-710 - 40 L; 30 T L: 85 J at RT
T: 55 J at RT AFNOR NF A 49-217:1987 TU Z 6 CND 17 11 - - HF + CR + Q (HY) - - 190 - 490-740 - 45 90 HRB max
Trang 13Handbook of Comparative World Steel Standards
5.9 Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures
5.9.2B Mechanical Properties of Austenitic Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures (Continued)
Thickness Yield Strength, min Tensile Strength, min Standard
Designation Grade, Class, Type, Symbol or Name Number Steel Number UNS Heat Treatment Product Form/ t, mm t, in N/mm 2 or
2 or
Elongation, min, % Other
T: 55 J at RT DIN 17457:1985 X 2 CrNiMo 18 14 3 1.4435 - SA & Q ≤ 50 - 190 - 490-690 - 40 L; 35 T L: 85 J at RT
T: 55 J at RT DIN 17458:1985 X 2 CrNiMo 18 14 3 1.4435 - SA & Q ≤ 50 - 190 - 490-690 - 40 L; 30 T L: 85 J at RT
T: 55 J at RT AFNOR NF A 49-217:1987 TU Z 2 CND 17 12 - - HF + CF + Q (HY) - - 175 - 470-720 - 45 90 HRB max
TU Z 2 CND 18 14 - - HF + CF + Q (HY) - - 210 - 490-690 - 45 - AFNOR NF A 49-247:1981 TS Z 2 CND 17-12 - - Q (HY) - - 215 - 520-720 - 40 -
Trang 14MPa MPa
DIN 17457:1985 X 2 CrNiMoN 17 13 3 1.4429 - SA & Q ≤ 50 - 295 - 580-800 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT DIN 17458:1985 X 2 CrNiMoN 17 13 3 1.4429 - SA & Q ≤ 50 - 295 - 580-800 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT AFNOR NF A 49-217:1987 TU Z 2 CND 17 12 AZ - - HF + CF +
BS 3605-1:1990 Issue 2, 1997 316S51 - - ST or HF - - 240 - 510-710 - 35 -
DIN 17459:1992 X 6 CrNiMo 17 13 1.4919 - SHT ≤ 50 - 205 - 490-690 - 35 L; 30 T L: 90 J at RT
T: 60 J at RT AFNOR NF A 49-214:1978 Z 6 CND 17-12 B - - L or F/H + RC - - 195 - 490-690 - 40 -
BS 3605-1:1990 Issue 2, 1997 316S52 - - ST or HF - - 240 - 510-710 - 35 -
DIN 17459:1992 X 3 CrNiMoN 17 13 1.4910 - SHT ≤ 50 - 260 - 550-750 - 35 L; 30 T L: 120 J at RT
T: 80 J at RT
Trang 15Handbook of Comparative World Steel Standards
5.9 Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures
5.9.2B Mechanical Properties of Austenitic Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures (Continued)
Thickness Yield Strength, min Tensile Strength, min Standard
Designation Grade, Class, Type, Symbol or Name Number Steel Number UNS Heat Treatment Product Form/ t, mm t, in N/mm 2 or
2 or
Elongation, min, % Other
T: 55 J at RT
≤ 50 - 210 - 500-730 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT DIN 17458:1985 X 6 CrNiMoTi 17 12 2 1.4571 - SA & Q
≤ 50 - 190 - 490-690 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT
SA & Q ≤ 50 - 210 - 500-730 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT DIN 28180:1985 X 6 CrNiMoTi 17 12 2 1.4571 -
SA & Q ≤ 50 - 190 - 490-690 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT DIN 28181:1985 X 6 CrNiMoTi 17 12 2 1.4571 - SA & Q ≤ 50 - 210 - 500-730 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT AFNOR NF A 49-214:1978 Z 8 CNDT 17-13 B - - L or F/H + RC - - 195 - 540-740 - 40 -
NOTE: This section continued on next page
Trang 16ASTM A 358/A 358M-01 321 - S32100 H, HT, HT-O
ASTM A 376/A 376M-02a TP321 - - see standard - ≤ ³⁄₈ 205 30 515 75 35 -
ASTM A 409/A 409M-01 TP321 - S32100 H, HT, HT-O
≤ 50 - 180 - 460-680 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT
SA & Q ≤ 50 - 200 - 500-730 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT DIN 28180:1985 X 6 CrNiTi 18 10 1.4541 -
SA & Q ≤ 50 - 180 - 460-680 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT DIN 28181:1985 X 6 CrNiTi 18 10 1.4541 - SA & Q ≤ 50 - 200 - 500-730 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT AFNOR NF A 49-217:1987 TU Z 6 CNT 18 10 - - HF + CR + Q (HY) - - 190 - 490-740 - 45 90 HRB max
Trang 17Handbook of Comparative World Steel Standards
5.9 Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures
5.9.2B Mechanical Properties of Austenitic Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures (Continued)
Thickness Yield Strength, min Tensile Strength, min Standard
Designation Grade, Class, Type, Symbol or Name Number Steel Number UNS Heat Treatment Product Form/ t, mm t, in N/mm 2 or
2 or
Elongation, min, % Other
ASTM A 312/A 312M-03 TP321H Welded - S32109 HF or CF + A - - 205 30 515 75 35 -
ASTM A 358/A 358M-01 347 - S34700 H, HT, HT-O
ASTM A 409/A 409M-01 TP347 - S34700 H, HT, HT-O
Trang 18MPa MPa
DIN 17457:1985 X 6 CrNiNb 18 10 1.4550 - SA & Q ≤ 50 - 205 - 510-740 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT DIN 17458:1985 X 6 CrNiNb 18 10 1.4550 - SA & Q ≤ 50 - 205 - 510-740 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT
BS 3605-1:1990 Issue 2, 1997 347S51 - - ST or HF - - 240 - 510-710 - 35 -
DIN 17459:1992 X 8 CrNiNb 16 13 1.4961 - SHT ≤ 50 - 205 - 510-690 - 35 L; 22 T 65 J at RT, L
45 J at RT, T AFNOR NF A 49-214:1978 Z 6 CN Nb 18-12 B - - L or F/H + RC - - 195 - 490-690 - 40 -
ASTM A 409/A 409M-01 - - S31725 H, HT, HT-O
DIN 17457:1985 X 2 CrNiMoN 17 13 5 1.4439 - SA & Q ≤ 50 - 285 - 580-800 - 35 L; 30 T L: 85 J at RT
T: 55 J at RT DIN 17458:1985 X 2 CrNiMoN 17 13 5 1.4439 - SA & Q ≤ 50 - 285 - 580-800 - 35 L; 30 T L: 85 J at RT
Trang 19Handbook of Comparative World Steel Standards
5.9 Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures
5.9.2B Mechanical Properties of Austenitic Stainless Steel Tubes and Pipes for Pressure Purposes and High Temperatures (Continued)
Thickness Yield Strength, min Tensile Strength, min Standard
Designation Grade, Class, Type, Symbol or Name Number Steel Number UNS Heat Treatment Product Form/ t, mm t, in N/mm 2 or
2 or
Elongation, min, % Other
ASTM A 358/A 358M-01 - - N08904 H, HT, HT-O
Trang 20A25 Class I - PSL 1 API 5L-2004
A25 CIass II - PSL 1 - - see standard - - 172 25 310 45 see standard - L175, Class I
ISO 3183-1:1996
API 5L-2004 A - PSL 1 - - see standard - - 207 30 331 48 see standard -
EN 10208-1:1997 L210GA 1.0319 - see standard - - 210 - 335-475 - 25 -
API 5L-2004 B - PSL 1 - - see standard - - 241 35 414 60 see standard -
CSA Z245.1-2002 241 - Category I - - see standard - - 241-495 - 414-760 - see standard -
EN 10208-1:1997 L245GA 1.0459 - see standard - - 245 - 415-555 - 22 -
API 5L-2004 X42 - PSL 1 - - see standard - - 290 42 414 60 see standard -
CSA Z245.1-2002 290 - Category I - - see standard - - 290-495 - 414-760 - see standard -
EN 10208-1:1997 L290GA 1.0483 - see standard - - 290 - 415-555 - 21 -
API 5L-2004 X46 - PSL 1 - - see standard - - 317 46 434 63 see standard -
CSA Z245.1-2002 317 - Category I - - see standard - - 317 - 434 - see standard -
API 5L-2004 X52 - PSL 1 - - see standard - - 359 52 455 66 see standard -
CSA Z245.1-2002 359 - Category I - - see standard - - 359-530 - 455-760 - see standard -
EN 10208-1:1997 L360GA 1.0499 - see standard - - 360 - 460-620 - 20 -
API 5L-2004 X56 - PSL 1 - - see standard - - 386 56 490 71 see standard -
CSA Z245.1-2002 386 - Category I - - see standard - - 386-540 - 490-760 - see standard -
API 5L-2004 X60 - PSL 1 - - see standard - - 414 60 517 75 see standard -
CSA Z245.1-2002 414 - Category I - - see standard - - 414-565 - 517-760 - see standard -
API 5L-2004 X65 - PSL 1 - - see standard - - 448 65 531 77 see standard -
CSA Z245.1-2002 448 - Category I - - see standard - - 448-600 - 531-760 - see standard -
API 5L-2004 X70 - PSL 1 - - see standard - - 483 70 565 82 see standard -
CSA Z245.1-2002 483 - Category I - - see standard - - 483-620 - 565-760 - see standard -
CSA Z245.1-2002 550 - Category I - - see standard - - 550-690 - 620-830 - see standard -
ISO 3183-1:1996 L555 - - see standard - - 555 - 625-825 - 15 27 J at 0°C
see standard